Documente Academic
Documente Profesional
Documente Cultură
: 3
Date: August 8, 1995 Revision Date: August 3, 2000
Supporting PQR No. (s): L5652 (PRN144), L10275 ( PRN144-1), & L10613 (PRN160 )
Welding Process: GTAW Type(s): Manual
This WPS must be used in-conjunction with WPS No. GEN.
JOINTS (QW-402)
Refer to WPS No. GEN for typical joint designs. This WPS is to be used with or without backing.
BASE METALS (QW-403)
Thickness Range:
.280 thru .750 With Impact Tests 9B31.3 at 150oF or higher)
Base Metal Groove 1/16 thru .750 W/O Impact Tests Fillets All
.625 Maximum w/o PWHT for ASME Section B31.1 and Section III Fabrication.
TECHNIQUE (QW-410)
Notes:
3) For impact tested fabrication only, minimum allowable travel speed shall be determined by the
following formula (fabrication without impact testing has no travel speed requirements):