Sunteți pe pagina 1din 8

TEST REPORT NUMBER : BGLT09002247

DATE : 16-Feb-2009

APPLICANT : MADURA GARMENTS EXPORTS LIMITED./BANGALORE


"MG HOUSE", SALARPURIA SENATE, NO.110, 4TH
CROSS, 5TH BLOCK,,KORAMANGALA INDUSTRIAL
LAYOUT,,BANGALORE,INDIA,560 095
ATTN : NUPUR.
CC : AMIT AHUJA,
Smriti Chand [Triburg-Bangalore],

Sample Description : MEN'S CARGO SHORTS


No. of Pieces of Garment : TWO
Product Type : CARGO SHORTS
Program : NOT PROVIDED
End Uses : CARGO SHORTS
Fabric Code : NOT PROVIDED
Description : TWO PIECES OF SUBMITTED WOVEN MEN'S CARGO
SHORTS WITH RELEVANT FABRIC SAID TO BE 100%
COTTON IN COLOR MARKED AS BLACK.
Sample Submitted are for : TESTING
Construction : 110 X 56
Fabric Name : NOT PROVIDED
Width : NOT PROVIDED
Contracted Weight : NOT PROVIDED
Fiber Content : 100% COTTON
Garment Supplier : MADURA GARMENTS EXPORTS LTD
Piece Goods Country of Origin : INDIA
Finishing Mill : ASHIMA
Piece Goods Supplier : NOT PROVIDED
Buyer Name : PHILLIPS-VAN HEUSEN
Division : CALVIN KLEIN SPORTSWEAR - MEN'S
Style No : 40WB627
Colour : BLACK
P.O. No. : --
Specification No. : --
Season : SUMMER'09
Pattern Number : NOT PROVIDED
Shipment Quantity : NOT PROVIDED
Ship Date : NOT PROVIDED
Purpose of Testing : WOVEN GARMENT PRIMARY PACKAGE
Type of Dye : NOT PROVIDED
Yarn Size/Gauze : 16S X 10S
Applicant Provided Care Instructions :
PC728
MACHINE WASH COLD
GENTLE CYCLE WITH LIKE COLORS
ONLY NON CHLORINE BLEACH WHEN NEEDED
TUMBLE DRY LOW
IRON LOW HEAT

PREPARED & CHECKED BY :


FOR INTERTEK TESTING SERVICES INDIA PRIVATE LTD. [BANGALORE]

KARTHIKEYAN C
LAB MANAGER

TEX/67 Page 1 of 8
Intertek Testing Services India Private Ltd.
17/F, Industrial Suburb, 2nd stage, Yeshwanthpur Industrial Area, Bangalore - 560022. Karnataka. India.
Tel : 080 - 40213700 Fax :080 - 40213960
Registered Office : G3, Ground Floor, Akruti Corporate Park, LBS Marg, Opp: Naval Civilian Housing Colony, Kanjurmarg (West), Mumbai – 400 079
Tel : +91-22-67976900., Fax : 91-22-5503 1087 Web site : www.intertek-labtest.com.
TEST REPORT NUMBER : BGLT09002247
DATE : 16-Feb-2009

Date Received/Date Test Started : 09 Feb 2009


Date Confirmation Received :-

TEST CONDUCTED : AS PER THE REQUEST OF THE APPLICANT. FOR FURTHER DETAILS PLEASE
REFER TO ENCLOSED PAGE(S)

CONCLUSION :
FIBRE IDENTIFICATION / COMPOSITION M
DIMENSIONAL STABILITY TO WASHING M
APPEARANCE AFTER WASH F1
SKEWING M
COLOR FASTNESS TO PERSPIRATION M
COLOR FASTNESS TO CROCKING M
COLOR FASTNESS TO NON-CHLORINE BLEACH M
COLOR FASTNESS TO LAUNDERING M
COLOR FASTNESS TO LIGHT M
COLOUR FASTNESS TO HEAT M
.FABRIC WEIGHT *
YARN COUNT M
FABRIC COUNT F2
PILLING RESISTANCE M
pH VALUE M
TENSILE STRENGTH AS RECEIVED M
TEAR STRENGTH M
SEAM SLIPPAGE/STRENGTH M
FLAMMABILITY TEST *
F1 = THE SUBMITTED SAMPLE FAILS IN APPEARANCE AFTER WASH BEING RESULT AS
AFTER THREE WASHES OBSERVATION : .:NOTICEABLE COATING REMOVAL OF
BUCKLE WAS OBSERVED [REQUIREMENT =]
AFTER THREE WASHES OBSERVATION : .:THE GENERAL APPEARANCE OF THE
WASHED GARMENT WAS NOT SATISFACTORY [REQUIREMENT =]
F2 = THE SUBMITTED SAMPLE FAILS IN FABRIC COUNT BEING RESULT AS
PER INCH WEFT:62 [REQUIREMENT =56]
NOTE : M = MEETS BUYER’S REQUIREMENT, F = BELOW BUYER’S REQUIREMENT
* = REQUIREMENT NOT PROVIDED, NA = NOT APPLICABLE
NOTE :
EXEMPTION 1:THE SUBMITTED SAMPLE IS EXEMPT FROM FLAMMABILITY TESTING SINCE FABRIC
WEIGHT EXCEEDS 2.6 OZ/SQ.YD AND IS A PLAIN SURFACE.

TEX/67 Page 2 of 8
Intertek Testing Services India Private Ltd.
17/F, Industrial Suburb, 2nd stage, Yeshwanthpur Industrial Area, Bangalore - 560022. Karnataka. India.
Tel : 080 - 40213700 Fax :080 - 40213960
Registered Office : G3, Ground Floor, Akruti Corporate Park, LBS Marg, Opp: Naval Civilian Housing Colony, Kanjurmarg (West), Mumbai – 400 079
Tel : +91-22-67976900., Fax : 91-22-5503 1087 Web site : www.intertek-labtest.com.
TEST REPORT NUMBER : BGLT09002247
DATE : 16-Feb-2009

TEST CONDUCTED (AS REQUESTED BY THE APPLICANT)


1. FIBRE IDENTIFICATION / COMPOSITION ¤
AATCC 20-2002/20A- 2000/2007
REQUIREMENT

WARP COTTON
WEFT COTTON
FIBRE COMPOSITION [ON FABRIC BASIS] :
: 100% COTTON 100%COTTON NO
TOLERANCE

2. DIMENSIONAL STABILITY TO WASHING ¤


AATCC 150-2003 TEST NO. (2)IIA(ii), 8 MIN MACHINE WASH AT 80 DEGREE F, GENTLE CYCLE
FOLLOWED BY TUMBLE DRY LOW WITH COOL IRON
UNRESTORED ORIGINAL [CM] AFTER 3RD DIMENSIONAL REQUIREMENT
WASH [CM] CHANGE (%)
SIDE SEAM 62.0 61.2 -1.3 4.0%
WAIST 43.0 42.5 -1.2
INSEAM 35.0 34.6 -1.1
FRONT RISE 28.2 28.1 -0.4
BACK RISE 43.2 43.0 -0.5
HIP 48.5 48.3 -0.4
LEG OPENING 28.0 27.9 -0.4
THIGH 35.0 34.6 -1.1
RESTORED ORIGINAL [CM] AFTER 3RD DIMENSIONAL REQUIREMENT
WASH [CM] CHANGE (%)
SIDE SEAM 62.0 60.7 -2.1 3.0%
WAIST 43.0 42.2 -1.9
INSEAM 35.0 34.4 -1.7
FRONT RISE 28.2 28.0 -0.7
BACK RISE 43.2 42.9 -0.7
HIP 48.5 48.1 -0.8
LEG OPENING 28.0 27.7 -1.1
THIGH 35.0 34.4 -1.7
REMARK:
(+) MEANS EXTENSION (-) MEANS SHRINKAGE

TEX/67 Page 3 of 8
Intertek Testing Services India Private Ltd.
17/F, Industrial Suburb, 2nd stage, Yeshwanthpur Industrial Area, Bangalore - 560022. Karnataka. India.
Tel : 080 - 40213700 Fax :080 - 40213960
Registered Office : G3, Ground Floor, Akruti Corporate Park, LBS Marg, Opp: Naval Civilian Housing Colony, Kanjurmarg (West), Mumbai – 400 079
Tel : +91-22-67976900., Fax : 91-22-5503 1087 Web site : www.intertek-labtest.com.
TEST REPORT NUMBER : BGLT09002247
DATE : 16-Feb-2009

3. APPEARANCE AFTER WASH


8 MIN MACHINE WASH AT 80 DEGREE F IN AATCC 1993 DETERGENT SOLUTION, GENTLE CYCLE
FOLLOWED BY TUMBLE DRY LOW WITH COOL IRON
AFTER THREE WASHES
REQUIREMENT
Colour Change 4
4
OBSERVATION
. SLIGHT COLOR CHANGE WAS OBSERVED
. NOTICEABLE COATING REMOVAL OF BUCKLE WAS OBSERVED
. SLIGHT FUZZINESS WAS OBSERVED
. NO PILLING WAS FOUND
. NO SKEWING WAS OBSERVED
. INITIALLY SEAM PUCKERS WERE OBSERVED WHICH INCREASED SLIGHTLY AFTER
WASH
. NO SEAM OPENING/BREAKAGE WAS OBSERVED
. NO DETERIORATION OF VELCRO WAS OBSERVED
. NO FRAYING/RAVELLING OF BUTTON HOLE TRIMS WAS OBSERVED
. NO COLOR LOSS/BREAKAGE OF BUTTON WAS OBSERVED
. NO LUSTER LOSS OF ZIPPER WAS OBSERVED
. FUNCTIONING OF ZIPPER WAS PROPER
. NO OBVIOUS SHAPE DISTORTION WAS OBSERVED
THE GENERAL APPEARANCE OF THE WASHED GARMENT WAS NOT SATISFACTORY

4. SKEWING
pvh sop 8 MIN MACHINE WASH AT 80 DEGREE F IN AATCC 1993 DETERGENT SOLUTION, GENTLE
CYCLE FOLLOWED BY TUMBLE DRY LOW WITH COOL IRON
REQUIREMENT
AFTER 3RD WASH NIL 4.0% OF THE
SIDE SEAM

5. COLOR FASTNESS TO PERSPIRATION


AATCC 15-2002
REQUIREMENT
COLOUR CHANGE 4-5 4
COLOUR STAINING ACETATE 4-5 4
COTTON 4-5
NYLON 4-5
POLYESTER 4-5
ACRYLIC 4-5
WOOL 4-5
SELF STAINING 4-5

TEX/67 Page 4 of 8
Intertek Testing Services India Private Ltd.
17/F, Industrial Suburb, 2nd stage, Yeshwanthpur Industrial Area, Bangalore - 560022. Karnataka. India.
Tel : 080 - 40213700 Fax :080 - 40213960
Registered Office : G3, Ground Floor, Akruti Corporate Park, LBS Marg, Opp: Naval Civilian Housing Colony, Kanjurmarg (West), Mumbai – 400 079
Tel : +91-22-67976900., Fax : 91-22-5503 1087 Web site : www.intertek-labtest.com.
TEST REPORT NUMBER : BGLT09002247
DATE : 16-Feb-2009

6. COLOR FASTNESS TO NON-CHLORINE BLEACH


SPOT WITH ONE DROPS OF 1.9% ULTRA CLOROX 2 AND WAIT FOR ONE MINUTE
BASE+ REQUIREMENT
POCKET
LINING
COLOUR CHANGE CLASS 4-5 4

7. COLOR FASTNESS TO CROCKING ¤


AATCC 8- 2001/2007
REQUIREMENT
DRY 3-4 3-4
WET 2-3 2-3

8. COLOR FASTNESS TO LAUNDERING ¤


AATCC 61- 2003/2007, [TEST NO. 2A, 45 MIN MECHANICAL WASH AT 120 DEGREE F, IN
0.15% AATCC WOB DETERGENT SOLUTION WITH 50 STEEL BALLS]
BASE+ REQUIREMENT
POCKET
LINING
COLOUR CHANGE 4 4
COLOUR STAINING ACETATE 4-5 3
COTTON 4-5
NYLON 4-5
POLYESTER 4-5
ACRYLIC 4-5
WOOL 4-5
SELF STAINING 4-5 4

9. COLOR FASTNESS TO LIGHT ¤


AATCC 16E-1998
REQUIREMENT

[10 AFU] COLOUR CHANGE 4-5 blank


CLASS --
[20 AFU] COLOUR CHANGE 4 4
CLASS

TEX/67 Page 5 of 8
Intertek Testing Services India Private Ltd.
17/F, Industrial Suburb, 2nd stage, Yeshwanthpur Industrial Area, Bangalore - 560022. Karnataka. India.
Tel : 080 - 40213700 Fax :080 - 40213960
Registered Office : G3, Ground Floor, Akruti Corporate Park, LBS Marg, Opp: Naval Civilian Housing Colony, Kanjurmarg (West), Mumbai – 400 079
Tel : +91-22-67976900., Fax : 91-22-5503 1087 Web site : www.intertek-labtest.com.
TEST REPORT NUMBER : BGLT09002247
DATE : 16-Feb-2009

10. COLOUR FASTNESS TO HEAT


AATCC 133- 1999/2004 CLASS IV] TEMP. USED [200 C 2]
REQUIREMENT
DRY PRESSING COLOUR 4-5 3
CHANGE
DAMP PRESSING COLOUR 4-5
CHANGE
STAINING 4-5
ON COTTON
WET PRESSING COLOUR 4-5
CHANGE
STAINING 3-4
ON COTTON
AFTER CONDITIONING
REQUIREMENT
DRY PRESSING COLOUR 4-5 3
CHANGE
DAMP PRESSING COLOUR 4-5
CHANGE
STAINING 4-5
ON COTTON
WET PRESSING COLOUR 4-5
CHANGE
STAINING 3-4
ON COTTON

11. .FABRIC WEIGHT ¤


ASTM D3776-1996 (2002)
REQUIREMENT
GM/SQ.MTR 337 Not Provided
OZ./SQ.YDS. 9.9

12. YARN COUNT


ASTM D1059 -2001
REQUIREMENT
WARP 15.5 Ne 16's
WEFT 9.6 Ne 10's
REMARK:
Ne = NEW ENGLISH COTTON COUNT
Tolerance:±5%

TEX/67 Page 6 of 8
Intertek Testing Services India Private Ltd.
17/F, Industrial Suburb, 2nd stage, Yeshwanthpur Industrial Area, Bangalore - 560022. Karnataka. India.
Tel : 080 - 40213700 Fax :080 - 40213960
Registered Office : G3, Ground Floor, Akruti Corporate Park, LBS Marg, Opp: Naval Civilian Housing Colony, Kanjurmarg (West), Mumbai – 400 079
Tel : +91-22-67976900., Fax : 91-22-5503 1087 Web site : www.intertek-labtest.com.
TEST REPORT NUMBER : BGLT09002247
DATE : 16-Feb-2009

13. FABRIC COUNT


ASTM D3775 - 2003/2007
PER INCH REQUIREMENT
WARP 116 110
WEFT 62 56
REMARK:
Tolerance:±5%

14. PILLING RESISTANCE ¤


ASTM D3514-2002 [AFTER 200 STROKES]
REQUIREMENT
RATING 4 3

15. pH VALUE
AATCC 81- 2001/2006
REQUIREMENT
7.9 6-8

16. TENSILE STRENGTH AS RECEIVED ¤


ASTM D5034-1995(2001) 1 Inch Grab Test, Tinius Olsen CRE
REQUIREMENT
WARP 108.1 lbf 50 lbf
WEFT 76.1 lbf

17. TEAR STRENGTH ¤


ASTM D1424- 1996/07, Elmendorf Tester
REQUIREMENT
WARP 106 oz 40 oz
WEFT 120 oz

TEX/67 Page 7 of 8
Intertek Testing Services India Private Ltd.
17/F, Industrial Suburb, 2nd stage, Yeshwanthpur Industrial Area, Bangalore - 560022. Karnataka. India.
Tel : 080 - 40213700 Fax :080 - 40213960
Registered Office : G3, Ground Floor, Akruti Corporate Park, LBS Marg, Opp: Naval Civilian Housing Colony, Kanjurmarg (West), Mumbai – 400 079
Tel : +91-22-67976900., Fax : 91-22-5503 1087 Web site : www.intertek-labtest.com.
TEST REPORT NUMBER : BGLT09002247
DATE : 16-Feb-2009

18. SEAM SLIPPAGE/STRENGTH ¤


ASTM D 434 –1995 /ASTM D 1683-1990
REQUIREMENT
S.O.@ 0.25” STRENGTH SLIPPAGE STRENGTH
SIDE SEAM [lbf] * 72.5 FR 15 lbf 25 lbf
FRONT ACROSS SEAM [lbf] * 89.0 FTS
INSEAM [lbf] * 73.0 FTS
BACK RISE SEAM [lbf] * 124.0 STB
REMARK:
* = THE SEAM OPENING WAS LESS THAN 0.25 INCH
FR = FABRIC RUPTURE
FTS = FABRIC TORN AT SEAM
STB = SEWING THREAD BROKEN

## END OF THE TEST REPORT ##

TEX/67 Page 8 of 8
Intertek Testing Services India Private Ltd.
17/F, Industrial Suburb, 2nd stage, Yeshwanthpur Industrial Area, Bangalore - 560022. Karnataka. India.
Tel : 080 - 40213700 Fax :080 - 40213960
Registered Office : G3, Ground Floor, Akruti Corporate Park, LBS Marg, Opp: Naval Civilian Housing Colony, Kanjurmarg (West), Mumbai – 400 079
Tel : +91-22-67976900., Fax : 91-22-5503 1087 Web site : www.intertek-labtest.com.