Sunteți pe pagina 1din 10

REFRACTORY MATERIAL PROPERTIES

▣ Indonesia Balikpapan RFCC Project


Licensor Recommendation Proposal
Refractory
Remarks
Type
Manufacturer Product Name Manufacturer Product Name Manufacturer Product Name

1A - - PLIBRICO PLIGUN LWI-24 RESCO RESCOCAST 9

- - PLIBRICO PLICAST LWI-22 RESCO RESCOCAST 3E


1B
- - PLIBRICO PLIGUN LWI-22 RESCO RESCOCAST 3E

PLIFLOW ABREST VF
2A-C DRAMICOM ACTCHEM 45 VC PLIBRICO RESCO RESCOCAST 17EC
(Former name : PLICAST ABREST)
PLIFLOW ABREST VF
2A-F DRAMICOM ACTCHEM 45 TF PLIBRICO RESCO SUREFLOE 17E
(Former name : PLIFLOW ABREST)

2A-G DRAMICOM ACTCHEM 45 GUNITE PLIBRICO PLIGUN ABREST RESCO RESCOCAST 17EG

PLIFLOW ABREST MW VF
2B-C CALDERYS CALDE CAST MW 148 CO HR PLIBRICO RESCO RESCOCAST 17EMC
(Former name : PLICAST ABREST MW)
PLIFLOW ABREST MW VF
2B-F CALDERYS CALDE FLOW MW 148 CO HR PLIBRICO RESCO SUREFLOE 17EM
(Former name : PLIFLOW ABREST MW)

2B-G CALDERYS CALDE GUN MW 148 CO HR PLIBRICO PLIGUN ABREST MW RESCO RESCOCAST 17EMG
CONFORMITY OF SPECFICATION
Refractory Material Equivalent to Axens Specification

Description AGC Plibrico RESCO

Axens Spec. Type 1A


PLIGUN LWI-24 RESCOCAST 9
Heat Insulating

Item Criteria Typical Data Typical Data

Maximum Service Temperature (℃) 1,100 1,350 1,427

Bulk Density (kg/m3)

After Drying at 110 ℃ 1,150 ~ 1,550 1,450 1,362

After Drying at 815 ℃ 1,150 ~ 1,450 1,350 1,201

Cold Crushing Strengh (kgf/cm2)

After Drying at 815 ℃ > 40 102 56 ~ 154

Erosion Loss (cm3)

After Drying at 815 ℃ - - -

Permanent Linear Change (%)

After Drying at 815 ℃ After drying at 110 ℃ basis) < -0.3 -0.2 0.0 ~ -0.3

Thermal Conductivity (W/mK)

At 815 ℃ < 0.45 0.44 0.44

Return Thermal Expansion (mm/m)

Between 540 ~ 815 ℃ 2.9 ~ 4.4 2.9 ~ 4.4

Installation Method - Pneumatic Gunite Pneumatic Gunite


CONFORMITY OF SPECFICATION
Refractory Material Equivalent to Axens Specification

Description AGC Plibrico RESCO

Axens Spec. Type 1B


PLICAST LWI-22 RESCOCAST 3E
Heat Insulating - Light Weight

Item Criteria Typical Data Typical Data

Maximum Service Temperature (℃) 1,100 1,200 1,205

Bulk Density (kg/m3)

After Drying at 110 ℃ 1,050 ~ 1,200 1,200 1,080

After Drying at 815 ℃ 970 ~ 1,200 1,100 976

Cold Crushing Strengh (kgf/cm2)

After Drying at 815 ℃ > 25 26 42 ~ 70

Erosion Loss (cm3)

After Drying at 815 ℃ - - -

Permanent Linear Change (%)

After Drying at 815 ℃ After drying at 110 ℃ basis) < -0.3 -0.2 -0.1 ~ -0.3

Thermal Conductivity (W/mK)

At 815 ℃ < 0.33 0.29 0.25

Return Thermal Expansion (mm/m)

Between 540 ~ 815 ℃ 2.9 ~ 4.4 2.9 ~ 4.4

Installation Method - Casting Casting


CONFORMITY OF SPECFICATION
Refractory Material Equivalent to Axens Specification

Description AGC Plibrico RESCO

Axens Spec. Type 1B


PLIGUN LWI-22 RESCOCAST 3E
Heat Insulating - Light Weight

Item Criteria Typical Data Typical Data

Maximum Service Temperature (℃) 1,100 1,200 1,205

Bulk Density (kg/m3)

After Drying at 110 ℃ 1,050 ~ 1,200 1,200


1,040 ~ 1,200
After Drying at 815 ℃ 970 ~ 1,200 1,100

Cold Crushing Strengh (kgf/cm2)

After Drying at 815 ℃ > 25 36 49 ~ 77

Erosion Loss (cm3)

After Drying at 815 ℃ - - -

Permanent Linear Change (%)

After Drying at 815 ℃ After drying at 110 ℃ basis) < -0.3 -0.25 -0.2 ~ -0.4

Thermal Conductivity (W/mK)

At 815 ℃ < 0.33 0.29 0.29

Return Thermal Expansion (mm/m)

Between 540 ~ 815 ℃ 2.9 ~ 4.4 2.9 ~ 4.4

Installation Method - Pneumatic Gunite Pneumatic Gunite


CONFORMITY OF SPECFICATION
Refractory Material Equivalent to Axens Specification

Description AGC Plibrico RESCO

Axens Spec. Type 2A-C PLIFLOW ABREST VF


(Former name : RESCOCAST 17EC
Medium Erosion Resistant / Heat-insulating PLICAST ABREST)
Item Criteria Typical Data Typical Data

Maximum Service Temperature (℃) 1,100 1,400 1,510

Bulk Density (kg/m3)

After Drying at 110 ℃ 2,120 ~ 2,250 2,250 2,192

After Drying at 815 ℃ 2,050 ~ 2,200 2,150 2,080

Cold Crushing Strengh (kgf/cm2)

After Drying at 815 ℃ > 560 816 560 ~ 770

Erosion Loss (cm3)

After Drying at 815 ℃ < 10 8 10 (Max)

Permanent Linear Change (%)

After Drying at 815 ℃ After drying at 110 ℃ basis) < -0.3 -0.05 0.0 ~ -0.3

Thermal Conductivity (W/mK)

At 815 ℃ < 1.02 1.00 1.15

Return Thermal Expansion (mm/m)

Between 540 ~ 815 ℃ 3.5 ~ 5.2 3.5 ~ 5.2

Installation Method Vibocast Vibocast Vibocast


CONFORMITY OF SPECFICATION
Refractory Material Equivalent to Axens Specification

Description AGC Plibrico RESCO

Axens Spec. Type 2A-F PLIFLOW ABREST VF


(Former name : SUREFLOW 17E
Medium Erosion Resistant / Heat-insulating PLIFLOW ABREST)
Item Criteria Typical Data Typical Data

Maximum Service Temperature (℃) 1,100 1,400 1,510

Bulk Density (kg/m3)

After Drying at 110 ℃ 2,150 ~ 2,250 2,250 2,243

After Drying at 815 ℃ 2,050 ~ 2,200 2,150 2,160

Cold Crushing Strengh (kgf/cm2)

After Drying at 815 ℃ > 620 816 630 ~ 840

Erosion Loss (cm3)

After Drying at 815 ℃ < 12 8 12 (Max)

Permanent Linear Change (%)

After Drying at 815 ℃ After drying at 110 ℃ basis) < -0.3 -0.05 0.0 ~ -0.3

Thermal Conductivity (W/mK)

At 815 ℃ < 1.02 1.00 1.16

Return Thermal Expansion (mm/m)

Between 540 ~ 815 ℃ 3.5 ~ 5.2 3.5 ~ 5.2

Installation Method Freeflow Casting Freeflow Casting Freeflow Casting


CONFORMITY OF SPECFICATION
Refractory Material Equivalent to Axens Specification

Description AGC Plibrico RESCO

Axens Spec. Type 2A-G


PLIGUN ABREST RESCOCAST 17EG
Medium Erosion Resistant / Heat-insulating

Item Criteria Typical Data Typical Data

Maximum Service Temperature (℃) 1,100 1,400 1,510

Bulk Density (kg/m3)

After Drying at 110 ℃ 2,220 ~ 2,400 2,250 2,256

After Drying at 815 ℃ 2,100 ~ 2,400 2,100 2,128

Cold Crushing Strengh (kgf/cm2)

After Drying at 815 ℃ > 520 561 475 ~ 910

Erosion Loss (cm3)

After Drying at 815 ℃ < 14 13 14 (Max)

Permanent Linear Change (%)

After Drying at 815 ℃ After drying at 110 ℃ basis) < -0.3 -0.2 0.0 ~ -0.3

Thermal Conductivity (W/mK)

At 815 ℃ < 1.02 1.00 1.18

Return Thermal Expansion (mm/m)

Between 540 ~ 815 ℃ 3.5 ~ 5.2 3.5 ~ 5.2

Installation Method Pneumatic Gunite Pneumatic Gunite Pneumatic Gunite


CONFORMITY OF SPECFICATION
Refractory Material Equivalent to Axens Specification

Description AGC Plibrico RESCO

Axens Spec. Type 2B-C PLIFLOW ABREST MW VF


(Former name : RESCOCAST 17EMC
Less Erosion Resistant / More Heat-insulating PLICAST ABREST MW)
Item Criteria Typical Data Typical Data

Maximum Service Temperature (℃) 1,100 1,300 1,370

Bulk Density (kg/m3)

After Drying at 110 ℃ 1,840 ~ 1,930 1,900 1,856

After Drying at 815 ℃ 1,750 ~ 1,850 1,800 1,762

Cold Crushing Strengh (kgf/cm2)

After Drying at 815 ℃ > 350 510 350 ~ 630

Erosion Loss (cm3)

After Drying at 815 ℃ < 18 14 18 (Max)

Permanent Linear Change (%)

After Drying at 815 ℃ After drying at 110 ℃ basis) < -0.3 -0.05 0.0 ~ -0.3

Thermal Conductivity (W/mK)

At 815 ℃ < 0.72 0.70 0.71

Return Thermal Expansion (mm/m)

Between 540 ~ 815 ℃ 3.5 ~ 5.2 3.5 ~ 5.2

Installation Method Vibocast Vibocast Vibocast


CONFORMITY OF SPECFICATION
Refractory Material Equivalent to Axens Specification

Description AGC Plibrico RESCO

Axens Spec. Type 2B-F PLIFLOW ABREST MW VF


(Former name : SUREFLOW 17EM
Less Erosion Resistant / More Heat-insulating PLIFLOW ABREST MW)
Item Criteria Typical Data Typical Data

Maximum Service Temperature (℃) 1,100 1,300 1,370

Bulk Density (kg/m3)

After Drying at 110 ℃ 1,840 ~ 1,930 1,900 1,922

After Drying at 815 ℃ 1,750 ~ 1,850 1,800 1,842

Cold Crushing Strengh (kgf/cm2)

After Drying at 815 ℃ > 340 510 455 ~ 595

Erosion Loss (cm3)

After Drying at 815 ℃ < 18 14 18 (Max)

Permanent Linear Change (%)

After Drying at 815 ℃ After drying at 110 ℃ basis) < -0.3 -0.05 0.0 ~ -0.3

Thermal Conductivity (W/mK)

At 815 ℃ < 0.72 0.70 0.71

Return Thermal Expansion (mm/m)

Between 540 ~ 815 ℃ 3.5 ~ 5.2 3.5 ~ 5.2

Installation Method Freeflow Casting Freeflow Casting Freeflow Casting


CONFORMITY OF SPECFICATION
Refractory Material Equivalent to Axens Specification

Description AGC Plibrico RESCO

Axens Spec. Type 2B-G


PLIGUN ABREST MW RESCOCAST 17EMG
Less Erosion Resistant / More Heat-insulating

Item Criteria Typical Data Typical Data

Maximum Service Temperature (℃) 1,100 1,350 1,370

Bulk Density (kg/m3)

After Drying at 110 ℃ 1,840 ~ 1,930 1,850 1,872

After Drying at 815 ℃ 1,750 ~ 1,850 1,750 1,792

Cold Crushing Strengh (kgf/cm2)

After Drying at 815 ℃ > 220 459 220 ~ 420

Erosion Loss (cm3)

After Drying at 815 ℃ < 20 14 14 (Max)

Permanent Linear Change (%)

After Drying at 815 ℃ After drying at 110 ℃ basis) < -0.3 -0.05 0.0 ~ -0.3

Thermal Conductivity (W/mK)

At 815 ℃ < 0.72 0.70 0.71

Return Thermal Expansion (mm/m)

Between 540 ~ 815 ℃ 3.5 ~ 5.2 3.5 ~ 5.2

Installation Method Pneumatic Gunite Pneumatic Gunite Pneumatic Gunite